Chemical Resistance Chart for Engineering Plastics: ABS, PC, Nylon, POM, PBT, PPS, PSU, PP & TPU Against Oils, Fuels, Acids & Solvents

A plastic part that passes every test in the lab can still crack in the field after a few weeks. Very often, the cause is a chemical: a cleaning spray, hand sanitiser, engine oil, a grease used during assembly, or petrol splashed on a fuel cap. Choosing a plastic that can handle the chemicals it will meet is just as important as choosing one that is strong enough.

At Jay Plast, we help OEMs and moulders choose materials for parts that come into contact with oils, fuels, cleaners, and solvents. This guide gives a chemical resistance chart for common engineering plastics, explains environmental stress cracking (the most common hidden failure), and shows which material to choose for common applications.


1. How Chemicals Damage Plastics

Chemicals can harm plastics in a few different ways:

  • Dissolving or swelling: Solvents such as acetone or toluene soften the surface, make it sticky, or dissolve it completely.
  • Chemical attack: Strong acids, strong alkalis, or hot water break the polymer chains. The part becomes weak and brittle. Breaking the chains with water is called hydrolysis.
  • Environmental Stress Cracking (ESC): A chemical that does no visible harm on its own causes cracks when the part is under stress. This is the most common chemical failure in real parts and is explained in Section 4.
  • Absorption: Some plastics, like nylon, absorb water and other liquids, which changes their size and stiffness.

As a general rule, semi-crystalline plastics (PP, nylon, POM, PBT, PPS) resist chemicals much better than amorphous plastics (ABS, PC, SAN, PSU). The tightly packed crystals make it hard for chemicals to get in.


2. Chemical Resistance Chart for Engineering Plastics

Key: G = Good (suitable), F = Fair (limited exposure only, test first), P = Poor (not recommended). Ratings are for room temperature.

ChemicalABSPC / PC+ABSSANNylon PA6 / PA66Nylon PA12POMPBTPPSPSU / PPSUPPTPU
Water (cold)GGGFGGGGGGG
Hot water / steamFPFFFGPGGGP
Dilute acidsGGGPFFGGGGF
Strong acidsFFFPPPFGGGP
Dilute alkalisGFGGGGFGGGF
Strong alkalisGPGFGGPGGGP
Oils and greasesFFGGGGGGGFG
Petrol / dieselPPFGGGGGFFG
Alcohols (IPA, ethanol)FFFFGGGGGGF
Ketones (acetone, MEK)PPPGGGFGPGP
Chlorinated solventsPPPFFFFGPPP
Aromatic solvents (toluene, xylene)PPPGGGFGPFF

General guidance only, based on typical unfilled grades. Results change with concentration, temperature, time, and stress. Always test the actual part in the actual chemical.


3. Notes by Material

  • ABS and SAN: Fine with water, dilute acids, and alkalis. Attacked by acetone, solvents, and petrol. ABS can stress crack with some oils and cleaners.
  • Polycarbonate and PC+ABS: Very tough but the most sensitive to chemicals among common engineering plastics. Attacked by solvents, petrol, strong alkalis, and ammonia. PC also hydrolyses in hot water and steam over time. It is very prone to stress cracking.
  • Nylon PA6 and PA66: Excellent with oils, greases, fuels, and most solvents, which is why nylon is widely used in automotive parts. Poor with acids. Absorbs water, which changes size and stiffness. Can crack when exposed to road salt (calcium chloride and zinc chloride).
  • Nylon 12: Like PA6 and PA66 but absorbs much less water and handles salts much better, making it the choice for fuel lines, air brake tubing, and under-bonnet tubes. See our Nylon 12 guide.
  • POM (Delrin / Acetal): Excellent with fuels, oils, and solvents. Copolymer grades handle hot water and alkalis well. Poor with acids and chlorine, so avoid POM in swimming pool equipment or chlorinated water systems with high chlorine levels.
  • PBT: Good with oils, fuels, and many solvents. Not suitable for long contact with hot water, steam, or strong alkalis because of hydrolysis.
  • PPS: Close to the best chemical resistance of any thermoplastic. No known solvent below 200°C. Used in pump parts, chemical processing, and fuel system parts.
  • PSU and PPSU: Excellent with hot water, steam, acids, and alkalis, so they are used in medical items that are sterilised and in hot water plumbing. Attacked by ketones and many solvents. PPSU is generally more resistant than PSU.
  • PP: Excellent with acids, alkalis, and water. Used for chemical tanks and battery cases. Swells in oils, fuels, and some solvents.
  • TPU: Excellent with oils, greases, and fuels, which is why it is used in hoses, seals, and cable jackets. Polyester-based TPU is weak in hot water. Choose polyether-based TPU for wet conditions.

4. Environmental Stress Cracking (ESC): The Hidden Failure

Environmental stress cracking happens when a chemical and stress act together. The chemical alone does no visible harm, and the stress alone is safe, but together they cause fine cracks that grow until the part breaks. This can happen weeks or months after the part leaves the factory.

Common causes of ESC in real products:

  • PC housings cracking around screw bosses after contact with hand sanitiser, alcohol wipes, or disinfectants.
  • ABS and PC parts cracking where assembly grease, thread-locking compounds, or anti-rust sprays have been used.
  • PC and PC+ABS cracking in contact with soft PVC cables, because plasticisers move from the PVC into the part.
  • ABS parts cracking from cleaning products or cooking oils in kitchen appliances.

Where does the stress come from?

  • Moulded-in stress from cold moulds, high injection speed, or over-packing.
  • Assembly stress from press fits, snap fits, inserts, and overtightened screws.
  • Load during use.

How to prevent ESC:

  1. Choose the right material. Semi-crystalline plastics like PBT, nylon, POM, and PPS are much more resistant to ESC than amorphous ones.
  2. Use a chemically resistant blend. PC+PBT blends combine the toughness of PC with the chemical resistance of PBT. They are widely used for automotive exterior parts. See our PC+PBT guide.
  3. Reduce moulded-in stress with a hotter mould, slower filling, and balanced packing.
  4. Design out stress points: add radii at sharp corners, avoid tight press fits, and control screw torque.
  5. Check every chemical the part will touch, including greases, cleaners, adhesives, and gaskets used during assembly.
  6. Test parts under stress in the actual chemical, not just flat samples without load.

5. Which Plastic to Choose for Common Applications

ApplicationChemicals InvolvedGood Choices
Fuel caps, fuel system partsPetrol, diesel, ethanol blendsPOM, PA12, PA66 GF, PPS
Under-bonnet automotive partsOil, coolant, brake fluid, road saltPA66 GF30, PA12, PBT GF30, PPS GF40
Medical device housingsDisinfectants, alcohol, sanitisersPC+PBT, PPSU, chemical-resistant PC grades (test first)
Kitchen appliance partsDetergents, oils, hot waterPP, PBT, POM
Hot water plumbing fittingsHot water, chlorinePPSU, PSU, PPS
Chemical tanks and battery casesAcids, alkalisPP
Hydraulic and pneumatic fittingsHydraulic oil, compressed airPOM, PA6 GF30, PA66
Cable jackets and hosesOils, greases, fuelsTPU (polyether for wet use)
Cosmetics and personal care packsOils, alcohols, fragrancesPP, SAN, PBT (test for ESC)

6. How to Test Chemical Resistance

  • Soak test: Soak samples in the chemical for a set time, then check weight change, size change, appearance, and strength.
  • Strained test (bent strip or jig test): Clamp a sample bent to a set strain and apply the chemical. Check for cracks after 24 hours to 1 week. This is the best simple test for ESC.
  • Real part test: Assemble the real part with real screws and inserts, apply the chemical, and age it at the highest use temperature.

Always test at the highest temperature the part will see. Chemical attack gets much faster as temperature rises.


7. Get the Right Material From Jay Plast

At Jay Plast, we supply engineering plastics for chemically demanding parts, including PC+PBT, PBT, nylon PA6, PA66, PA12, POM, PPS, PSU, PPSU, PP, and TPU. Tell us what chemicals your part will meet, and our team will suggest suitable grades, share data sheets, and help you with samples for testing.

Based in Mumbai, we supply OEMs and moulders in Maharashtra, Gujarat, Delhi NCR, Tamil Nadu, Karnataka, and across India.

Contact Jay Plast today to find a chemically resistant grade for your part and get competitive per-kg pricing!