How to Dry Engineering Plastics Before Moulding: Drying Temperature & Time Chart for PC, ABS, Nylon, PBT, POM, PPS & More
Ask any experienced moulder what causes the most rejected parts, and many will say the same thing: wet material. Silver streaks, bubbles, brittle parts, poor surface finish, and cracked snap-fits are very often caused by granules that were not dried properly before moulding.
This is especially true in India, where monsoon humidity can stay above 80% for weeks. Material that moulded perfectly in winter can suddenly start giving rejects in July.
At Jay Plast, we supply engineering plastics including PC, ABS, nylon, PBT, POM, PPS, PSU, and TPU. In this guide, we explain which plastics need drying, how long to dry them, which dryer to use, and how to check that your material is really dry.
1. Why Drying Matters
Some plastics absorb water from the air. These are called hygroscopic plastics. Others only collect a little moisture on the surface.
When wet hygroscopic material is melted, two things can happen:
- The water turns to steam, causing silver streaks, bubbles, and splay on the surface.
- The water breaks the polymer chains (hydrolysis). This is the more serious problem. Polycarbonate, PBT, and PET are especially sensitive. The part may look fine but be much weaker and more brittle than it should be.
Damage from hydrolysis cannot be reversed. Once the polymer chains are broken in the barrel, the part is permanently weaker.
2. Drying Chart for Common Engineering Plastics
| Material | Drying Temperature | Drying Time | Target Moisture | Dryer Type |
|---|---|---|---|---|
| ABS | 80°C–85°C | 2–4 hours | < 0.1% | Desiccant (hot air OK in dry weather) |
| SAN | 75°C–85°C | 2–3 hours | < 0.05% | Desiccant |
| Polycarbonate (PC) | 120°C | 3–4 hours | < 0.02% | Desiccant |
| PC+ABS | 100°C–110°C | 3–4 hours | < 0.02% | Desiccant |
| PC+PBT | 110°C–120°C | 3–4 hours | < 0.02% | Desiccant |
| PBT | 120°C | 3–4 hours | < 0.02% | Desiccant |
| Nylon PA6 / PA66 | 80°C | 4–6 hours | 0.1%–0.2% | Desiccant or vacuum |
| Nylon 12 | 80°C | 4 hours | < 0.1% | Desiccant or vacuum |
| POM (Delrin) | 80°C–100°C | 2–3 hours | < 0.2% | Hot air or desiccant |
| TPU | 90°C–110°C | 2–3 hours | < 0.05% | Desiccant |
| PPS | 140°C | 3–4 hours | < 0.05% | Desiccant |
| PSU | 135°C–150°C | 3–4 hours | < 0.02% | Desiccant |
| PPSU | 150°C | 3–4 hours | < 0.02% | Desiccant |
| PP, PE, POE | Usually not needed | (80°C for 1 hour if surface moisture) | – | Hot air |
These are typical values. Always follow the data sheet for your specific grade.
3. Choosing the Right Dryer
A. Hot Air Dryer
Blows heated room air through the material. It is cheap and simple, but room air in India is often very humid, so it cannot dry hygroscopic plastics to low moisture levels. Suitable for removing surface moisture from PP, PE, and POM, and for ABS in dry weather.
B. Desiccant (Dehumidifying) Dryer
Passes air through a desiccant bed that removes moisture, then heats the dry air and blows it through the material. Good desiccant dryers deliver air with a dew point of -40°C or lower. This is the standard choice for PC, PBT, nylon, PPS, PSU, TPU, and blends.
C. Vacuum Dryer
Lowers the pressure so water boils off at lower temperatures. Dries material much faster and is useful for nylon and other materials that can yellow if heated too long in air.
D. Compressed-Air Dryer
Uses dried compressed air. Good for small machines and low throughput, especially in micro-moulding.
4. Sizing Your Dryer Hopper
The material must stay in the hopper for the full drying time. A simple rule:
Hopper capacity (kg) = Machine throughput (kg/hour) × Drying time (hours) × 1.2
Example: A machine using 25 kg/hour of polycarbonate, which needs 4 hours of drying: 25 × 4 × 1.2 = 120 kg hopper capacity.
If the hopper is too small, material passes through before it is fully dry, even if the temperature setting is correct.
5. Common Drying Mistakes
- Using a hot air dryer for PC or PBT in the monsoon. The material will not reach 0.02%, no matter how long you dry it.
- Drying for too long or too hot. Over-drying can turn nylon yellow, damage FR additives, and cause POM to give off odour. Most materials should not stay at drying temperature for more than 8–12 hours.
- Leaving dried material in an open hopper or container. PC and nylon can pick up moisture again in 30 minutes to 1 hour in humid weather.
- Saturated desiccant. If the dryer is not regenerating properly, the dew point rises and drying stops working. Check the dew point meter regularly.
- Forgetting to dry regrind. Regrind has more surface area and can be wetter than virgin granules.
- Blocked filters. Dirty filters reduce airflow and drying efficiency.
6. How to Check That Material Is Dry
- Moisture analyser: Weighs a sample, heats it, and measures the weight lost. The most reliable method for most shops.
- TVI (Tomasetti Volatile Indicator) test: Press a few hot granules between two glass slides. Many bubbles mean the material is wet. A quick, cheap check on the shop floor.
- Dew point meter on the dryer: Confirms the dryer is supplying dry air (aim for -40°C).
- Part checks: Silver streaks near the gate or brittle snap-fits are warning signs.
7. Storing Granules Correctly
- Keep bags sealed until use, and reseal part-used bags tightly.
- Store material off the floor and away from walls, in a dry, covered area.
- Do not store bags in direct sun or near open doors during the monsoon.
- Use first-in, first-out stock rotation.
8. Source Engineering Plastics and Technical Support from Jay Plast
At Jay Plast, we supply PC, ABS, PC+ABS, nylon, PBT, POM, PPS, PSU, PPSU, TPU, and more, in properly sealed packaging. Our team can help you set drying conditions for each grade and troubleshoot moisture-related defects.
We serve injection moulders and extruders in Mumbai, Pune, Gujarat, Delhi NCR, Chennai, Bangalore, and across India.
Contact Jay Plast today for data sheets with drying conditions, technical support, and competitive bulk pricing!