Injection Moulding Shrinkage Chart: Shrinkage Rates for ABS, PC, Nylon, POM, PBT, PP & Glass-Filled Plastics, Plus How to Control Warpage
Every plastic shrinks as it cools in the mould. A part that is 100 mm in the tool might come out at 99.5 mm with one material and 98 mm with another. Toolmakers cut moulds slightly oversize to allow for this. If the shrinkage is predicted wrongly, or if you change to a material that shrinks differently, the part comes out undersized, warped, or impossible to assemble.
At Jay Plast, we often help moulders who want to switch grades or brands without changing their tool. In this guide, we give a shrinkage chart for common engineering plastics, explain what makes shrinkage go up or down, and share practical tips to control warpage.
1. Why Plastics Shrink
Hot molten plastic takes up more space than cold solid plastic. As it cools in the mould, it contracts. How much it contracts depends mainly on the type of polymer:
- Amorphous plastics (ABS, PC, PC+ABS, SAN, PSU, PPSU) have a random molecular structure. They shrink less and more evenly, usually 0.3%–0.8%.
- Semi-crystalline plastics (PP, PE, nylon, POM, PBT, PPS) form tightly packed crystals as they cool. They shrink more, usually 1.0%–2.5%, and are more likely to warp.
Adding glass fibre or mineral filler greatly reduces shrinkage, but glass fibres make shrinkage different along the flow and across the flow, which is a common cause of warpage.
2. Mould Shrinkage Chart for Common Plastics
| Material | Type | Typical Shrinkage (%) |
|---|---|---|
| SAN | Amorphous | 0.3–0.5 |
| ABS | Amorphous | 0.4–0.7 |
| Polycarbonate (PC) | Amorphous | 0.5–0.7 |
| PC+ABS | Amorphous blend | 0.5–0.7 |
| PSU / PPSU | Amorphous | 0.6–0.8 |
| PC+PBT | Blend | 0.8–1.2 |
| TPU | Elastomer | 0.8–1.5 (varies with hardness) |
| Nylon PA6 | Semi-crystalline | 1.0–1.5 |
| Nylon PA66 | Semi-crystalline | 1.2–2.0 |
| Nylon 12 | Semi-crystalline | 1.0–2.0 |
| PP (Homopolymer / Copolymer) | Semi-crystalline | 1.2–2.0 |
| PBT | Semi-crystalline | 1.5–2.0 |
| HDPE | Semi-crystalline | 1.5–3.0 |
| POM (Delrin / Acetal) | Semi-crystalline | 1.8–2.5 |
| PA6 / PA66 GF30 | Glass-filled | 0.3–0.5 (flow), 0.8–1.2 (across) |
| PBT GF30 | Glass-filled | 0.3–0.6 (flow), 0.8–1.2 (across) |
| PPS GF40 | Glass-filled | 0.2–0.4 (flow), 0.4–0.8 (across) |
| PP Talc-Filled (20%–40%) | Mineral-filled | 0.8–1.2 |
Typical ranges for general guidance. Always use the value on your grade's data sheet for tool design.
3. What Makes Shrinkage Go Up or Down
Even with the same material, shrinkage changes with part design and moulding settings:
| Factor | Effect on Shrinkage |
|---|---|
| Thicker walls | More shrinkage (slower cooling, more crystals form) |
| Higher packing pressure | Less shrinkage (more material packed in) |
| Longer packing / hold time | Less shrinkage (until the gate freezes) |
| Larger gate | Less shrinkage (gate stays open longer for packing) |
| Higher mould temperature | More shrinkage in the mould for semi-crystalline plastics, but less shrinkage after moulding |
| Higher melt temperature | Usually slightly more shrinkage |
| Glass fibre or filler | Much less shrinkage, but different along and across the flow |
| Distance from gate | Areas far from the gate often shrink more (less packing pressure reaches them) |
4. Post-Mould Shrinkage: Measure at the Right Time
Some plastics keep shrinking for days after moulding as crystals continue to form. This is called post-mould shrinkage. It is most noticeable in POM, PP, PBT, and PE, especially if they were moulded in a cold mould.
Tip: Measure critical dimensions 24 to 48 hours after moulding, not straight off the machine. For precision POM gears, a warmer mould (80°C–100°C) gives more stable dimensions over the life of the part.
Nylon is different: after moulding, PA6 and PA66 absorb moisture from the air and grow slightly. Account for this when designing tight-fitting nylon parts. Nylon 12 grows much less.
5. Warpage: When Shrinkage Is Uneven
A part warps when one area shrinks more than another. Common causes and fixes:
- Uneven wall thickness: Thick areas shrink more than thin ones. Design walls as evenly as possible, and core out thick sections.
- Uneven mould cooling: If one side of the tool is hotter, that side shrinks more. Balance cooling channels and check water flow.
- Glass fibre orientation: Fibres line up with the flow. Move the gate or use a lower glass content if warpage is severe.
- Not enough packing: Increase pack pressure and time so the whole part is packed evenly.
- Ejecting too early: Parts that are too hot when ejected continue to move. Increase cooling time.
6. Switching Materials Without Changing the Tool
Moulders often want to switch to a cheaper grade, a different brand, or reprocessed material. Before switching:
- Stay in the same material family. Switching from ABS to PC+ABS usually works. Switching from ABS to PP will not.
- Compare shrinkage on both data sheets, using the same test method.
- Check filler content. A GF30 grade will not fit a tool cut for GF15 or unfilled material.
- Run trial parts and measure them after 24–48 hours before approving.
7. Talk to Jay Plast Before You Switch Grades
At Jay Plast, we supply ABS, PC, PC+ABS, SAN, nylon, PBT, POM, PPS, PSU, PPSU, TPU, and more, in both virgin and reprocessed grades. Our team can help you find a grade that matches the shrinkage of your current material, so your tool keeps producing good parts.
We support injection moulders in Mumbai, Pune, Gujarat, Delhi NCR, Chennai, Bangalore, and across India.
Contact Jay Plast today for data sheets, grade matching advice, and samples for trial runs!