Injection Moulding Clamping Force Calculation: Tonnage Chart for ABS, PC, Nylon, POM, PBT, PPS & How to Choose the Right Machine
"Which tonnage machine do I need for this mould?" is one of the first questions in any injection moulding job. With too little clamping force, the mould opens slightly during injection and you get flash. With far more than you need, you pay for a bigger machine, crush the mould vents, and put extra wear on the tool.
At Jay Plast, we often help moulders when a new material changes how a job runs. This guide explains how to calculate clamping force, gives tonnage factors for common engineering plastics, and shows what else to check before you put a mould on a machine.
1. What Is Clamping Force?
During injection, molten plastic pushes against the mould with very high pressure. That pressure tries to force the two mould halves apart. Clamping force is the force the machine applies to keep them shut.
In India, machine size is commonly given in tonnes (T), such as a 150T or 250T machine.
2. The Clamping Force Formula
Clamping force (tonnes) = Total projected area (cm²) × Tonnage factor (t/cm²)
The tonnage factor depends on the material and represents the average pressure inside the cavity. For example, 0.45 t/cm² is the same as 450 kg/cm², or about 44 MPa.
If you prefer to work in kN:
Clamping force (kN) = Projected area (cm²) × Cavity pressure (MPa) ÷ 10
One tonne-force is about 9.81 kN.
3. How to Find the Projected Area
Projected area is the shadow of the part when you look straight along the direction the mould opens. Depth does not count, so a tall cup and a flat disc of the same diameter have the same projected area.
- Rectangular part: Length × Width
- Round part: 3.14 × Radius²
- Multi-cavity mould: Area of one part × Number of cavities
- Add the runner: Include the projected area of the runner and sprue
- Through holes: You can subtract large holes that are fully shut off in the mould
Most CAD software can measure this directly.
4. Clamping Force Chart by Material
| Material | Starting Tonnage Factor (t/cm²) |
|---|---|
| TPU | 0.25–0.45 |
| PP | 0.30–0.45 |
| HDPE | 0.30–0.45 |
| ABS / SAN | 0.35–0.55 |
| Nylon PA6 / PA66 | 0.35–0.60 |
| PC+ABS | 0.40–0.60 |
| PBT | 0.40–0.60 |
| POM (Delrin / Acetal) | 0.45–0.70 |
| Polycarbonate (PC) | 0.50–0.75 |
| PA6 / PA66 GF30 | 0.50–0.75 |
| PBT GF30 | 0.50–0.75 |
| PPS GF40 | 0.50–0.80 |
| PSU / PPSU | 0.60–0.90 |
These are starting estimates for typical parts. Grade, flow length, wall thickness, and gate design all affect the real pressure. For critical jobs, use mould flow simulation.
How to pick a value in the range:
- Use the lower end for easy-flow grades, thick walls, and short flow lengths.
- Use the higher end for stiff-flowing grades, thin walls, long flow lengths, and tight tolerances.
5. Correct for Thin Walls
Thin walls need much higher injection pressure. Multiply your result by a wall thickness factor:
| Nominal Wall Thickness | Multiply By |
|---|---|
| Above 2.5 mm | 1.0 |
| 1.5–2.5 mm | 1.0–1.2 |
| 1.0–1.5 mm | 1.2–1.5 |
| Below 1.0 mm | 1.5 or more (run a flow simulation) |
Also check the flow length to wall thickness ratio. A part that has a 200 mm flow path and a 1 mm wall has a ratio of 200:1, which is demanding for many engineering plastics. The melt flow index of your grade gives a first idea of how easily it flows.
6. Worked Example
A rectangular cover measures 150 mm × 100 mm with a 2.5 mm wall. The mould has 2 cavities, and the runner adds 20 cm².
Step 1: Projected area
- One part: 15 cm × 10 cm = 150 cm²
- Two cavities: 150 × 2 = 300 cm²
- With runner: 300 + 20 = 320 cm²
Step 2: Clamping force and machine selection
| Material | Factor | Force (320 × Factor) | With 15% Safety Margin | Suggested Machine |
|---|---|---|---|---|
| PP | 0.35 | 112 T | 128.8 T | 150T |
| ABS | 0.45 | 144 T | 165.6 T | 180T |
| PC | 0.65 | 208 T | 239.2 T | 250T |
This shows why changing material can change the machine you need. The same mould that runs comfortably on a 150T machine in PP may need a 250T machine in PC.
7. Tonnage Is Not the Only Machine Check
A machine with enough clamping force may still not fit the job. Check these too:
| Check | What to Confirm |
|---|---|
| Tie-bar spacing | The mould fits between the tie bars, or can be loaded from the side |
| Mould height | Mould thickness is between the machine's minimum and maximum |
| Opening stroke | Enough to eject the part and runner and let them fall or be picked out |
| Shot capacity | Shot uses about 20%–80% of barrel capacity |
| Injection pressure | Enough for the material and wall thickness |
| Ejector stroke | Enough to fully clear the part |
| Mould temperature | Machine setup can reach the required temperature, especially for PPS, PSU, and PPSU |
For target temperatures by material, see our injection moulding temperature chart.
8. How to Set the Right Clamp on the Machine
Running at maximum clamp "to be safe" is a common and costly habit. Too much clamp can:
- Close the vents, causing burn marks and short shots
- Damage parting lines, which leads to permanent flash
- Bend platens and tie bars over time
- Waste energy and shorten machine and mould life
A simple shop-floor method:
- Fill and pack the part at your normal settings.
- Reduce clamping force step by step until a small amount of flash just appears.
- Increase clamping force by about 10% above this point.
- Check that parts stay flash-free over a production run.
9. Troubleshooting Flash and Clamp Problems
| Symptom | Likely Cause | What to Do |
|---|---|---|
| Flash all around the parting line | Clamp too low, or packing too high | Reduce packing first, then increase clamp if needed |
| Flash on one side only | Mould or platens not parallel, or mould off-centre | Centre the mould and check platen parallelism |
| Flash in one area of the tool | Worn or damaged shut-off | Inspect and repair the mould |
| Burn marks at the end of fill | Vents crushed or blocked | Reduce clamp and clean the vents |
| Flash only with a new lot or grade | Higher-flow material | Check MFI and adjust melt temperature and packing |
For more help, read our injection moulding defects guide.
10. Get Grade and Processing Support From Jay Plast
At Jay Plast, we supply ABS, PC, PC+ABS, SAN, nylon PA6, PA66, PA12, glass-filled grades, PBT, POM, PPS, PSU, PPSU, TPU, and POE, with full data sheets. If a part is close to your machine's limit, our team can help you look at a higher-flow grade that may reduce the pressure needed.
Based in Mumbai, we supply injection moulders in Maharashtra, Gujarat, Delhi NCR, Tamil Nadu, Karnataka, and across India.
Contact Jay Plast today for the right grade, technical support, and competitive per-kg pricing!