Injection Moulding Temperature Chart: Melt and Mould Temperatures for ABS, PC, Nylon, POM, PBT, PPS, PSU & More
Getting the temperature right is the first step to a good moulded part. If the melt is too cold, the material will not fill the mould, and you get short shots, flow lines, and weak weld lines. If it is too hot, the polymer breaks down, and you get burn marks, black specks, splay, brittle parts, and in some cases dangerous gases. The mould temperature matters just as much. It controls surface finish, shrinkage, warpage, and how strong the part is.
At Jay Plast, moulders often ask us for starting temperatures when they try a new material or grade. In this guide, we give a melt and mould temperature chart for common engineering plastics, explain how to set your barrel zones, and share tips on what to change when parts are not coming out right.
1. Melt Temperature vs Mould Temperature
- Melt temperature is the actual temperature of the molten plastic as it leaves the nozzle. It is not the same as the barrel heater set points. Screw speed and back pressure add extra heat through friction, so the real melt is often 5–20°C hotter or colder than the settings suggest.
- Mould temperature is the temperature of the steel surface that touches the part. It is controlled by water or oil running through the mould's cooling channels, using a mould temperature controller (MTC) or chiller.
Both need to be inside the right window for the material. The data sheet for your grade gives the recommended range, and it is always the best starting point.
2. Injection Moulding Temperature Chart
| Material | Melt Temperature (°C) | Mould Temperature (°C) | Max Melt Temp to Avoid (°C) |
|---|---|---|---|
| PP (Homopolymer / Copolymer) | 200–250 | 20–50 | ~280 |
| HDPE | 200–260 | 20–60 | ~290 |
| TPU | 190–230 (depends on hardness) | 20–50 | ~240 |
| POM (Delrin / Acetal) Copolymer | 185–210 | 60–100 | ~230 |
| SAN | 210–260 | 40–80 | ~280 |
| ABS | 220–260 | 40–80 | ~280 |
| Nylon 12 (PA12) | 230–270 | 40–80 | ~290 |
| PC+ABS | 250–280 | 60–90 | ~290 |
| PBT | 240–270 | 60–90 | ~280 |
| PBT GF30 | 250–275 | 70–110 | ~285 |
| PC+PBT (Xenoy-type blends) | 250–280 | 60–80 | ~290 |
| Nylon PA6 | 230–270 | 60–90 | ~290 |
| Nylon PA6 GF30 | 260–290 | 80–100 | ~300 |
| Nylon PA66 | 270–295 | 60–90 | ~305 |
| Nylon PA66 GF30 | 280–305 | 80–110 | ~310 |
| Polycarbonate (PC) | 280–320 | 80–110 | ~330 |
| PPS GF40 | 300–330 | 130–150 | ~345 |
| PSU (Polysulfone) | 330–370 | 120–160 | ~390 |
| PPSU | 350–390 | 140–170 | ~400 |
Typical ranges for general guidance. Always follow the data sheet for your exact grade. Flame-retardant (FR) grades often need lower melt temperatures than the standard grade.
3. How to Set Your Barrel Zones
Most machines have 3–5 heater zones plus the nozzle. A normal setup is a rising profile, cooler at the feed throat and hotter towards the nozzle:
| Zone | Typical Setting |
|---|---|
| Feed throat | Water-cooled, 40–60°C, so granules do not stick and bridge |
| Rear zone (feed) | 20–30°C below the target melt temperature |
| Middle zone (compression) | 10–15°C below target |
| Front zone (metering) | At target melt temperature |
| Nozzle | At target, or 5–10°C below for materials that drool |
When to use a flat or reverse profile:
- Long residence time (small shot on a big barrel): use a flatter, cooler profile to reduce degradation.
- Glass-filled grades and high-viscosity materials: a slightly hotter rear zone can reduce screw torque and fibre breakage.
Residence time matters too. Aim to use 20%–80% of the barrel's shot capacity. If the shot is very small, the plastic sits in the hot barrel for too long and starts to degrade, even if the set temperatures are correct. This is especially important for POM, PC, and FR grades.
4. How to Measure the Real Melt Temperature
Set points only tell you what the heaters are aiming for. To check the real melt temperature:
- Retract the nozzle and purge a shot into an insulated cup or onto a clean surface.
- Put a pre-heated needle probe pyrometer into the middle of the purge straight away.
- Move the probe slowly until the reading stops rising.
- Compare the reading with the data sheet range.
For mould temperature, use a surface contact probe on both halves of the mould after a few cycles. The cavity and core often run at different temperatures, which is a common cause of warpage.
5. Why Mould Temperature Matters
For amorphous plastics (ABS, PC, PC+ABS, SAN, PSU, PPSU):
- A hotter mould gives better gloss, fewer flow lines, weaker visible weld lines, and lower moulded-in stress.
- A colder mould gives faster cycles but more stress, which can lead to cracking later, especially with PC and PSU.
For semi-crystalline plastics (PP, nylon, POM, PBT, PPS):
- The mould must be hot enough for proper crystallisation. If it is too cold, the part may look fine but will keep shrinking and warping after moulding, and properties like stiffness and heat resistance will be lower.
- PPS is the extreme case. It needs a mould at 130°C or more, which means an oil or pressurised-water heater, not a normal water MTC.
- Glass-filled grades need a hotter mould to get a smooth surface and stop glass fibres showing on the part.
6. Material-Specific Warnings
- POM (Delrin / Acetal): Never overheat or leave it sitting in a hot barrel. POM breaks down into formaldehyde gas, which is harmful and can build pressure in the barrel. Purge thoroughly, and never mix POM with PVC in the same barrel.
- Polycarbonate: Very sensitive to moisture. Wet PC at 300°C will hydrolyse, causing splay, bubbles, and brittle parts. Dry it properly first. See our drying guide for engineering plastics.
- Nylon: Has a narrow processing window and drools easily. Use a shut-off nozzle or reverse taper, and keep it dry.
- FR grades (ABS FR, PC FR, PBT FR): Flame-retardant additives can break down at high temperatures and cause corrosion, black specks, and gas marks. Stay at the low to middle part of the melt range.
- PSU / PPSU and PPS: Need high temperatures, so check that your heater bands, nozzle, and hot runner are rated for 350–400°C.
- TPU: Soft grades run cooler than hard grades. Overheating causes bubbles and a sticky surface.
7. Troubleshooting by Temperature
| Problem | Melt Temperature Change | Mould Temperature Change |
|---|---|---|
| Short shots | Increase | Increase |
| Flow lines / poor gloss | Increase | Increase |
| Visible weld lines | Increase | Increase |
| Burn marks / black specks | Decrease (and reduce residence time) | No change |
| Splay / silver streaks | Decrease (and check drying) | No change |
| Flash | Decrease | Decrease |
| Sink marks | Decrease slightly | Decrease |
| Warpage | Small effect | Balance the cavity and core temperatures |
| Brittle parts | Check for overheating and wet material | Increase for semi-crystalline plastics |
| Sticking in the mould | Decrease | Decrease |
For more on fixing defects, read our injection moulding defects troubleshooting guide.
8. Get Processing Support From Jay Plast
At Jay Plast, we supply ABS, PC, PC+ABS, SAN, nylon PA6, PA66, PA12, glass-filled grades, PBT, POM, PPS, PSU, PPSU, TPU, and POE, along with full data sheets and recommended processing settings. If you are moving to a new grade or brand, our team can help you with starting temperatures, drying, and trials.
Based in Mumbai, we supply injection moulders in Maharashtra, Gujarat, Delhi NCR, Tamil Nadu, Karnataka, and across India.
Contact Jay Plast today for the right grade, full processing data, and competitive per-kg pricing!