Plastic Heat Resistance Chart: HDT, Continuous Use Temperature & Melting Points for ABS, PC, Nylon, PBT, PPS, PSU & PPSU
"How hot can this plastic take?" is one of the most common questions we hear. The answer is not one number. A plastic can survive a short burst of heat that would ruin it over months, and a part that holds its shape when unloaded may bend at the same temperature when it carries a load. Many failures in kettles, LED drivers, motor housings, and under-bonnet parts happen because the wrong heat number was used to select the material.
At Jay Plast, we supply engineering plastics for heat-exposed parts across India. In this guide, we give a heat resistance chart for common plastics, explain the different temperature numbers on a data sheet, and show which material to choose for each temperature range.
1. The Heat Numbers You Need to Know
| Term | What It Means | Use It For |
|---|---|---|
| HDT (Heat Deflection Temperature) | The temperature at which a test bar bends a set amount under a fixed load (0.45 MPa or 1.8 MPa) | Comparing how well materials hold their shape under load for a short time |
| Vicat Softening Point | The temperature at which a needle sinks 1 mm into the plastic under load | Comparing softening, mainly for amorphous plastics |
| Continuous Use Temperature / RTI | The temperature a material can handle for a long time (often 100,000 hours) and still keep at least half of its properties | Long-term use, electrical parts, and UL approvals |
| Glass Transition Temperature (Tg) | The temperature at which an amorphous plastic changes from stiff and glassy to soft and rubbery | The practical upper limit for amorphous plastics |
| Melting Point (Tm) | The temperature at which the crystals in a semi-crystalline plastic melt | The absolute upper limit for semi-crystalline plastics |
The key point: HDT tells you about short-term heat under load. Continuous use temperature tells you about long-term heat ageing. A part that runs hot all day needs to be selected on continuous use temperature, not HDT. To learn more about these values on a data sheet, read our guide to reading a plastic TDS.
2. Heat Resistance Chart for Plastics
| Material | HDT at 1.8 MPa (°C) | Continuous Use Temp (°C) | Tg / Melting Point (°C) |
|---|---|---|---|
| HDPE | 45–50 | 70–80 | Tm ~130 |
| PP (Homopolymer) | 55–65 | 90–100 | Tm ~165 |
| PP Talc-Filled (20%–40%) | 70–90 | 100–110 | Tm ~165 |
| Nylon 12 (PA12) | 45–55 | 80–90 | Tm ~178 |
| PBT (Unfilled) | 55–65 | 120–130 | Tm ~225 |
| Nylon PA6 (Unfilled, dry) | 60–75 | 80–100 | Tm ~220 |
| Nylon PA66 (Unfilled, dry) | 70–100 | 90–110 | Tm ~260 |
| SAN | 85–100 | 60–80 | Tg ~105 |
| ABS (General Purpose) | 80–95 | 60–80 | Tg ~105 |
| ABS (Heat Resistant) | 95–110 | 80–90 | Tg ~115–120 |
| POM (Delrin / Acetal) | 95–110 | 90–100 | Tm ~165–175 |
| PC+PBT | 90–110 | 90–110 | Mixed |
| PC+ABS | 95–115 | 80–100 | Tg ~110–135 |
| Polycarbonate (PC) | 125–135 | 115–125 | Tg ~145–150 |
| PSU (Polysulfone) | 170–175 | 150–160 | Tg ~185 |
| Nylon PA6 GF30 | 190–210 | 110–130 | Tm ~220 |
| PBT GF30 | 200–210 | 130–140 | Tm ~225 |
| PPSU | 205–210 | 160–180 | Tg ~220 |
| Nylon PA66 GF30 | 240–255 | 120–140 (heat-stabilised grades) | Tm ~260 |
| PPS GF40 | 260+ | 200–220 | Tm ~280 |
| TPU | Not used (soft material) | 80–100 | Varies |
Typical values for general guidance. Values vary by grade, colour, additives, and test method. Always check the data sheet for your exact grade.
3. Why Glass Fibre Changes Everything for Semi-Crystalline Plastics
Look at the chart again. Unfilled PBT has an HDT of about 60°C, but PBT GF30 jumps to over 200°C. Unfilled PA66 is around 70–100°C, but PA66 GF30 reaches 240–255°C. Why?
- In semi-crystalline plastics, the crystals stay solid up to the melting point, but the parts between the crystals soften at a much lower temperature. On their own, the bars bend early under load.
- Glass fibres act like a skeleton that holds everything together, so the part keeps its shape almost up to the melting point.
- In amorphous plastics like ABS and PC, adding glass fibre raises HDT only a little, because the whole material softens at the Tg.
This is why glass-filled nylon, PBT, and PPS are the standard choice for parts near engines, heaters, and motors. For more, see our glass-filled nylon guide.
But remember: a high HDT does not mean the material can stay at that temperature for years. PA66 GF30 has an HDT of around 250°C, but its continuous use temperature is only about 120–140°C, because heat slowly oxidises and weakens it over time. For long-term heat, choose heat-stabilised grades.
4. Short-Term vs Long-Term Heat
- Short peaks: Many plastics can handle short peaks 20–40°C above their continuous rating, such as during paint baking, a short overload, or a hot car parked in the sun.
- Long-term heat: Constant heat slowly breaks down the polymer by thermal oxidation. The part becomes brittle, changes colour, and loses impact strength.
- Under load: If the part carries a load, it can slowly bend or creep at temperatures well below the HDT. Design for the highest temperature and the highest load together.
- Electrical parts: For electrical products, the RTI (Relative Thermal Index) from UL is used. It is given separately for electrical, mechanical with impact, and mechanical without impact properties. See our UL94 flame ratings guide for other electrical safety ratings.
5. Which Plastic to Choose by Temperature
| Temperature Range | Typical Applications | Suitable Materials |
|---|---|---|
| Up to 70°C | Consumer goods, toys, housings, furniture parts | PP, ABS, SAN, HDPE |
| 70–100°C | Appliance housings, car interiors, hot-fill containers | Heat-resistant ABS, PC+ABS, POM, PP talc-filled |
| 100–130°C | LED lighting, electrical enclosures, kettles and coffee machine parts, car dashboards | PC, PBT, PC+PBT, PA6 GF30 |
| 130–150°C | Motor housings, connectors, switchgear, lamp holders | PBT GF30, PA66 GF30 (heat-stabilised), PSU |
| 150–180°C | Medical items sterilised by steam, hot water fittings, food service | PSU, PPSU |
| 180–220°C | Under-bonnet parts near the engine, electrical parts near heat sources, pump parts | PPS GF40 |
6. Tips for Heat-Exposed Parts
- Select on continuous use temperature, not just HDT, for parts that run hot all the time.
- Add a safety margin of 10–20°C above the highest expected temperature.
- Mould semi-crystalline parts in a hot enough mould. A cold mould gives low crystallinity, and the part will shrink and warp when it first heats up in use.
- Dry nylon parts before testing heat performance, or test conditioned parts, as moisture changes properties.
- Test the real part at the real temperature with the real load, for the real time. Heat ageing tests in an oven for 500–1,000 hours are common.
- Watch out for colour: some pigments, especially in FR grades, can reduce heat resistance or discolour at high temperatures.
7. Find a Heat-Resistant Grade at Jay Plast
At Jay Plast, we supply heat-resistant engineering plastics including heat-resistant ABS, PC, PC+ABS, PC+PBT, PBT and PBT GF30, nylon PA6 and PA66 GF30, POM, PPS GF40, PSU, and PPSU. Tell us the temperature, load, and life your part needs, and we will suggest the right grade and share full data sheets.
Based in Mumbai, we supply OEMs and moulders in Maharashtra, Gujarat, Delhi NCR, Tamil Nadu, Karnataka, and across India.
Contact Jay Plast today for heat-resistant grades, technical support, and competitive per-kg pricing!